https://mf.mw1950.com/cn/article/pdf/preview/44bc06dc-bc20-4d33-9d3f-775d78c75196.pdf 按此文獻電流值可為0.2A/sqin
似乎工藝如下。溫度68-70F。先去油超聲波洗淨;Lye按4湯匙:2Qt杯水比例混合做亞光蝕刻劑,浸泡0.5-2分鍾(視頻2水量加倍5分鍾);pHDown(So4)按30湯匙:8杯水比例混合做酸蝕劑(視頻2/3用電瓶水與水1:3浸5分鍾),用鋁板或其它導電金屬做陰極15-16V恒流4A (6A/Ft²?)電泳60分鍾,注意會冒泡;衝洗後放入120-140F的染色劑dye-royal-blue中15-20分鍾-此步可選;稍清洗後放入沸水鍋或封閉劑15分鍾。Hard Anodize將溫度降至 45°C,24 V電壓下60到90分鍾。